保(bao)溫瓶的香蕉視頻app在線觀看:不銹鋼外(wai)殼(ke)是由厚度(du)0.3~0.4mm的321不銹鋼超薄(bo)板卷制焊接而成。對接焊縫(feng)(feng)(feng)(feng)長度(du)270mm,正面(mian)焊縫(feng)(feng)(feng)(feng)熔寬小于(yu)2mm,焊縫(feng)(feng)(feng)(feng)余高在(zai)0.2mm下。焊縫(feng)(feng)(feng)(feng)不得有塌陷、燒(shao)穿(chuan)等缺陷,焊縫(feng)(feng)(feng)(feng)的首位(wei)端4mm以內允許有部分未焊透存在(zai)。采(cai)用微束香蕉視頻app在線觀看:等離子弧焊工藝,用胎(tai)夾具裝配獲(huo)得優(you)良的焊(han)(han)接(jie)(jie)接(jie)(jie)頭,焊(han)(han)縫成(cheng)形美觀,有較高的焊(han)(han)接(jie)(jie)生產(chan)率(lv)(lv),每45秒(miao)可(ke)焊(han)(han)接(jie)(jie)一(yi)個不銹鋼保溫(wen)瓶外殼,產(chan)品成(cheng)品率(lv)(lv)可(ke)達(da)95%.
1. 焊(han)前準備
按工藝要求(qiu)進(jin)行(xing)下料和卷(juan)筒,卷(juan)筒時注意將(jiang)邊緣(yuan)有毛刺的面向外。然后將(jiang)保(bao)溫瓶外殼待焊處(兩側各10mm)除去油污、銹,用丙酮擦干凈。由于不銹鋼的導熱(re)性能差,焊件(jian)又極薄,焊接時容(rong)易(yi)出現燒穿(chuan)和變(bian)形。焊接必須(xu)在胎夾具上進(jin)行(xing),即將(jiang)焊件(jian)緊緊地壓(ya)在銅墊板上進(jin)行(xing)焊接。
2. 焊接工(gong)藝
采用微束等離(li)子(zi)弧自動焊工藝。焊槍(qiang)噴嘴(zui)(zui)尺寸為:壓縮角90°,噴嘴(zui)(zui)孔(kong)徑1.0mm,噴嘴(zui)(zui)孔(kong)道長(chang)度1.0~1.2mm.鎢(wu)極選用2%的(de)鈰鎢(wu)電極,直徑1.5mm,端(duan)部呈錐狀,鎢(wu)極內(nei)縮量為0.8~1.0mm.
噴(pen)嘴(zui)距(ju)工件(jian)距(ju)離0.8~1.2mm。
經試驗(yan)后推薦的不銹鋼(gang)保(bao)溫瓶(ping)外殼(ke)脈(mo)沖微束等離子焊的工藝參(can)數見表5-1。
基本電流(liu)值為(wei)(wei)5A,脈沖占空比為(wei)(wei)60%左右,脈沖頻率為(wei)(wei)12~15Hz.焊(han)(han)縫的焊(han)(han)點重疊率為(wei)(wei)50%。